(1)
Rung Brill Blue 3G Pdr. Dyeing for Fabrics
Padding Process :
4 Parts
Ingrain Brill Blue 3G Pdr.
8 Parts Solvent Cum Emulsifier
10 Parts Urea
20 Parts Water followed
by addition of
50 Parts Ice cold Water
& Add
8 Parts Copper Complex
100 Parts
Pad and dry the material at about 80-90°C.
Cure at 150°C for about 5 to 6 minutes.
After treatment:
The material is rinse in cold water &
is treated with Sodium nitrite 4 gms/litre
& 5 gms/litre HCL at "boil for 20
minutes. Wash with Soap & Soda ash at
boil and rinse.(Without Guarantee)
(2) Rung Brill Blue
3G Pdr. Printing for Fabrics
Padding Process :
4 Parts
Ingrain Brill Blue 3G Pdr.
10 Parts Urea
20 Parts Water
8 Parts Copper Complex after
Stirring add
58 Parts gum thickening
100 Parts
Print on screen and dry in
air. Steam for one hour wash with cold water
and dry. (Without Guarantee)
(3) Rung Brill Blue
3GM Pdr. (Mixed with Copper Complex) \ Dyeing
for Fabrics
Padding Process :
6 Parts
Ingrain Brill Blue 3GM Pdr
8 Parts Solvent cum Emulsifier
10 Parts Urea
25 Parts followed by addition
of
51 Parts Ice cold water
100 Parts
Pad and dry the material
at about 80-90°C. Cure at 150°C for
about 5 to 6 minutes.
After treatment: The material
is rinse in cold water & is treated with
Sodium nitrite 4 gms/litre & 5 gms/litre
HCL at boil for 20 minutes. Wash with Soap
& Soda ash at boil and rinse. (Without
Guarantee)
(4) Rung Blue 3GM
Pdr. Printing for Fabrics
Padding Process :
6 Parts
Ingrain Brill Blue 3GM Pdr.
10 Parts Urea
26 Parts Water
58 Parts Gum Thickening
100 Parts
Print on screen and dry in
air. Steam for one hour wash with cold wat^r
and dry.
(5) Rung Blue 5
Application Printing
Application Printing:
Cellulose and silk. Dissolve in an organic
acid and thickaning and a spl. auxiliary agent
having reducing properties. Print, dry develop
with neutral or acid steam or by backing treat
in a hot acid bath. Rinse and Soap.
Can be printed alongside
azoic, reactive and vat dye and pigment and
on grounds of azoic coupling components.
(6) Rung Brill Blue
3GK Pdr. for Yarn Dyeing
MORDANTING (For 5 gm. Yarn)
The Yarn is soaped with Soda
Ash for 10-15 minutes at boil then rinse will.
200 mgm.
Mordant B.
150 CC.
Water at 70°C. Yarn is entered in Mordanting
bath After 10 minutes add. 1.5
gm. Glauber
Salt keep the yarn for 20 minutes in this
bath then after
squeezing take it to the dye bath.
DYE BATH (BEAKER SHOULD BE ABSOLUTELY DRY)
200 mgm.
Ingrain Brill. Blue 3GK.
400 mgm.
Diethylene Glycol.
1 gm.
Acetic Acid Glacial after
keeping the above for 20 minutes in cold
bath it is to be poured into
150 cc.
Ice Cold Water enter the Mordanted yarn into
this 'dye bath and
keep
it for 25 minutes. The dyed yarn is taken
out and developed in.
500 mgm.
Caustic Soda add.
300 mgm.
Sodium Hydrosulphite
100 cc.
Water at 60°C for 10 minutes the yarn
is stirred and then treated
with.
1 cc.
HCL
500 mgm. Sodium
Nitrite
100 cc. Water
at 60°C the yarn is kept for treatment
for 10 minutes.
The yarn rinsed in cold water
and washed with soap and soda ash at boil.
(Without Guarantee)
|